Root-Cause Analysis of Batch Longitudinal Cracking in API 6A Inconel 718 Hollow Bars During Forging

Company News

Hunan Shiney Steel Co., Ltd
Inconel 718,Hollow Bars,API 6A Inconel 718 Bar

Root-Cause Analysis of Batch Longitudinal Cracking in API 6A Inconel 718 Hollow Bars During Forging

Date:2026-11-23

Abstract

A batch of 27 API 6A Inconel 718 (N07718) nickel-alloy hollow bars exhibited extensive longitudinal surface cracks after forging and solution treatment. A multidisciplinary investigation combining defect morphology review, raw-material verification, forging-process document review, and shop-floor production assessment concluded that the cracking was not caused by ingot quality. Instead, the batch failure originated from unreasonable forging-process design and insufficient intermediate quality control. The main risk factors were an excessively high first-pass upsetting ratio, a final forging temperature below the material’s brittle-transition range, insufficient low-temperature holding for a large cross-section, and the absence of mandatory intermediate crack inspection and grinding. This article summarizes the investigation findings, root causes, corrective process parameters, quality-control improvements, and emergency disposition measures.

1. Incident Background

On 7 January 2026, quality inspectors tracking the production progress of 27 API 6A Inconel 718 (N07718) nickel-alloy hollow bars found that all 27 bars, after forging and solution treatment, showed longitudinal surface cracks to varying degrees. The event constituted a batch quality incident, resulting in delivery delay, material loss, and increased production cost. On 8 January 2026, technical and quality personnel visited the production site to conduct field verification, sampling review, and process traceability analysis.

2. Defect Morphology

All 27 forged and solution-treated bars were inspected individually. The defects had the following characteristics:

  • Crack morphology:Numerous irregular longitudinal linear cracks were distributed on the bar surfaces. Crack depth varied considerably, from approximately 0.3–1 mm in shallow cases to 3–5 mm at the deepest. Some cracks were accompanied by surface peeling.

  • Crack location:Cracks were concentrated in the middle section of the bars and in shoulder regions where stress concentration is expected. The two ends of the bars remained sound, with no exposed shrinkage cavities, elemental segregation, or inclusions.

  • Preliminary inference:The crack locations coincided closely with forging-stress concentration zones, indicating that the defects were highly likely induced by forging stress rather than by ingot-end or machining-related origins.

Inconel 718,Hollow Bars,API 6A Inconel 718 Bar

3. Raw-Material Verification

The full inspection reports for the vacuum arc remelted (VAR) ingots used for this batch were reviewed from five perspectives: chemical composition, gas content, metallographic structure, inclusions, and mechanical properties.

  1. Chemical composition:Spectrum analysis of the VAR ingots showed that both major alloying elements and trace elements met the Inconel 718 technical specification.

  2. Gas content:Hydrogen, oxygen, and nitrogen were controlled within a total of 40 ppm, and there was no gas-related internal porosity.

  3. The γ′ and γ″ strengthening phases were present as small amounts of dispersed precipitates—i.e., fine and dispersed—without chain-like or linear dense precipitation. No grain-boundary oxidation or abnormal grain coarsening was observed.

  4. Nonmetallic inclusions:No large harmful nonmetallic inclusions were detected.

  5. Mechanical properties:Tensile properties and impact energy of the same-heat samples all met the technical specification.

The raw-material verification therefore concluded that the ingot quality was acceptable. No abnormality was found in chemistry, gas content, microstructure, inclusions, or mechanical properties. The cracking was unrelated to the base material and originated from the forging process.

Inconel 718,Hollow Bars,API 6A Inconel 718 Bar

4. Forging Process and Production Review

4.1 Process Card Issues

A review of the forging process cards against the forging characteristics of Inconel 718 identified four key process concerns.

  1. Excessive first-pass upsetting deformation:The first upset reduced the billet height from 1200 mm to 700 mm, giving an upsetting ratio of 1.71. This single-pass deformation imposed a high forging load and generated significant internal residual stress. The process was corrected to leave the post-upset height at 850–900 mm to reduce single-pass deformation.

  2. Missing defect handling during forging:The process did not mandate crack inspection between forging passes. Small surface cracks were therefore not removed by grinding in time and could propagate during subsequent upsetting and drawing operations, eventually developing into deep cracks.

  3. Low final forging temperature:The final forging temperature for this batch was set at 850°C. The brittle-transition temperature of Inconel 718 is approximately 900°C; therefore, 850°C lies within the brittle range, where material plasticity decreases significantly and residual stress cannot be effectively released. This parameter required experimental verification and correction.

  4. Insufficient low-temperature holding:For a large cross-section bar of Ø252 mm, the low thermal conductivity of nickel-based alloys makes temperature uniformity difficult to achieve. The actual low-temperature holding time was about 1 h, while the process required ≥0.5 h. Although the actual time exceeded the minimum requirement, it was still insufficient to homogenize the section temperature; local regions cooled further, increasing cracking risk. The holding schedule therefore required revalidation.

Inconel 718,Hollow Bars,API 6A Inconel 718 Bar

4.2 Equipment and Shop-Floor Conditions

The workshop was equipped with an 8000-ton hydraulic forging press and ancillary air and electric hammers. All heating furnaces used natural gas. The hardware capability was adequate for forging this specification of nickel-alloy bar, and equipment was not considered a main cause of cracking.

Production records showed that white cracks appeared on the surface during forging. This observation supported the conclusion that cracking initiated during forging rather than during subsequent processing.

Inconel 718,Hollow Bars,API 6A Inconel 718 Bar

5. Comprehensive Root-Cause Analysis

Based on defect morphology, material testing, and process review, the batch longitudinal cracking was attributed to the following causal chain:

  1. Direct cause:The first-pass upsetting ratio was too large. Excessive compression generated high forging residual stress and provided the stress condition for crack initiation.

  2. Important contributing causes:The final forging temperature fell within the brittle range, and large-section holding was insufficient. The final temperature of 850°C was below the approximately 900°C brittle-transition temperature of Inconel 718. Combined with the poor thermal conductivity of nickel alloys and inadequate low-temperature holding, the bar cross-section developed a nonuniform temperature distribution. Local plasticity deteriorated, and longitudinal cracks initiated under residual stress.

  3. Management amplification factor:Intermediate quality control was missing. There was no mandatory crack inspection, grinding, and recording between forging passes. Early microcracks were not detected and removed, so they continued to propagate during subsequent forging deformation and developed into batch deep cracks.

In summary, the raw material was defect-free. The combination of high residual stress from an unreasonable forging process and low-temperature plasticity deterioration initiated the cracks, while the absence of in-process inspection allowed small cracks to develop into batch-rejectable defects.

6. Process Optimization and Quality Improvement

6.1 Forging Parameter Optimization

  • First-pass upsetting:Change the post-upset height from 700 mm to 850–900 mm to reduce the single-pass upsetting ratio and lower forging residual stress. The revised complete forging process document must be submitted for customer technical review by 14 January 2026.

  • Final forging temperature:Raise and control the final forging temperature to 900–930°C, with an absolute minimum of 900°C, to avoid the brittle-transition range and maintain material plasticity at the end of forging.

  • Low-temperature holding:For large-section billets, the low-temperature holding time should be ≥1 h to ensure temperature uniformity through the cross-section. At the same time, the upper holding limit must be strictly controlled to prevent grain coarsening; the finished grain size must meet the requirement of ≤3 grade.

6.2 Forging Quality-Control System

  • Implement the three-inspection system—self-inspection, mutual inspection, and dedicated inspection—and fully record the heating curve, actual deformation parameters, and crack-inspection results for each forging pass to establish a traceable process record.

  • Apply mandatory non-destructive testing at key operations: after upsetting and after drawing, perform 100% magnetic particle testing (MT) and confirm the absence of surface cracks before transferring to the next operation.

  • Establish a crack-grinding ledger recording crack location, grinding depth, operator, and re-inspection result. All ground areas must pass re-inspection.

6.3 Process Validation

After all process documents are revised, a small-batch trial forging must be conducted. Trial forgings must pass visual inspection, MT, and metallographic examination with no cracking risk before mass production is resumed.

7. Emergency Disposition

To reduce delivery losses, the following measures were implemented for the already produced blanks:

  1. Blank sorting and disposition:Five Ø178 billets were to be produced by turning from existing Ø250 billets with good surface quality. The remaining cracked blanks were to be returned for VAR remelting. For Ø240 forged blanks, the forging outer diameter was enlarged to approximately Ø265 to leave sufficient machining allowance. Two already produced Ø185 semi-finished bars must pass penetrant testing (PT) to confirm the absence of microcracks before continuing machining to the final Ø178 size.

  2. Emergency material input:Five backup ingots were selected for diffusion annealing, with furnace discharge planned for 15 January 2026, followed by emergency forging to support order delivery.

  3. Management closure:The new complete forging process card may be officially used only after customer technical review and confirmation.

8. Conclusions and Preventive Recommendations

  1. The batch longitudinal cracking of Inconel 718 hollow bars was not a raw-material quality problem.

  2. The root cause was forging-process design deficiency: excessive first-pass upsetting deformation, final forging temperature within the brittle range, insufficient low-temperature holding for a large cross-section, and missing intermediate crack inspection and grinding control. Together, these factors produced batch longitudinal stress cracks.

  3. For Inconel 718 nickel-based superalloy forging, the brittle-transition temperature must be fully considered, the lower limit of final forging temperature must be strictly controlled, and temperature uniformity in large-section billets must be emphasized. Experience with ordinary carbon steel or stainless steel cannot be directly applied.

  4. For large-deformation forging operations, the single-pass upsetting and drawing ratios must be strictly controlled to avoid excessive residual stress.

  5. MT must be embedded in key operations such as upsetting and drawing so that process defects can be detected and addressed early, preventing microcracks from propagating.

  6. New or revised processes must undergo small-batch trial validation before mass production.