IN792 and IN738LC belong to the same generation of cast γ′-strengthened nickel-base superalloys, yet they are not interchangeable. The decisive difference is one ofdesign intent: IN792 pushes the γ′ solvus higher and trades chromium for tantalum and tungsten to gain elevated-temperature strength, while IN738LC keeps a higher chromium level and a lower carbon specification to deliver mature, corrosion-resistant service in industrial gas turbines. Both have been the “norm in land-based gas turbines” for decades, and both remain difficult to weld or additively manufacture. The choice between them is therefore rarely about which alloy is “better” in the abstract; it is about which side of the strength–corrosion–processability triangle a given duty cycle actually needs.
The two alloys share the same Ni–Cr–Co–Mo–W–Al–Ti–Ta architectural framework, but the balance among the refractory and γ′-forming elements diverges sharply.
| Element (wt%, nominal) | IN738LC | IN792 |
|---|---|---|
| Cr | ~16 | ~12.5 |
| Co | ~8.5–8.6 | ~9.0 |
| W | ~2.5–2.6 | ~4.2–5.0 |
| Mo | ~1.7–1.8 | ~1.8–2.0 |
| Al | ~3.4–3.5 | ~3.4–3.5 |
| Ti | ~3.4–3.8 | ~4.2–3.9 |
| Ta | ~1.7–1.8 | ~4.0–4.2 |
| C | ~0.1 (low-carbon) | 0.016–0.21 adjustable |
Composition data from patent EP2425029A1 and corroborating sources.
The trade is explicit in the refractory balance. IN792 carries roughlytwice the tantalumof IN738LC (≈4 wt% versus ≈1.7 wt%) and a higher tungsten level. Ta and W partition in ways that raise the stability and volume fraction of the γ′ phase at temperature, which is the microstructural origin of IN792’s creep advantage. IN738LC, by contrast, retainsabout 16 wt% Cr versus ~12.5 wt% in IN792—a difference that directly sets their relative standing in hot corrosion. IN738LC’s “LC” designation refers to its low-carbon specification, which improves ductility and fatigue behavior relative to the standard carbon version.
The single most consequential thermal number is theγ′ solvus. IN792’s γ′ solvus sits near 1235 °C, above that of IN738LC. A higher solvus means the strengthening precipitate remains thermodynamically stable to a higher temperature before dissolving, so IN792 retains its strengthening architecture deeper into the creep regime.
The melting characteristics tell a complementary story. IN738LC exhibits awider melting interval(roughly 124 °C), which implies a greater propensity for segregation during solidification. IN792 solidifies over anarrower interval(roughly 82 °C), giving more concentrated solidification behavior and, in practice, a tighter process window for casting sound material. IN792 also has a higher solidus, consistent with its higher refractory content.
The compositional bet on Ta and W pays off increep and stress-rupture resistance. Comparative assessments place IN792 in the “high” creep-strength band among this alloy class, while IN738LC is not positioned at that extreme. In strain-controlled cyclic testing at 800 °C, IN792-5A develops ahigher stress amplitude than IN738LC at approximately the same total strain amplitude, and the difference is attributed to the significantly higher effective stress of its γ′ phase. That is a direct mechanical signature of a stronger precipitate–matrix interaction under load.
For designers, the practical translation is that IN792 is the alloy to specify when the metal temperature and stress combination pushes beyond what IN738LC can tolerate in long-term creep, particularly in gas turbine hot-section components where inlet temperatures are moving upward.
IN738LC’s higher chromium content buys it a clear advantage inhot corrosion resistance. A widely cited alloy-development assessment classifies hot corrosion resistance as“good” for IN738LC and “moderate” for IN792, explicitly attributing the ranking to chromium content. In fuels containing sulfur and vanadium—conditions not uncommon in industrial gas turbines burning lower-quality fuels—this difference is not academic. IN738LC has been the blade material of choice for industrial gas turbine hot-stage components precisely because it pairs adequate creep strength with reliable corrosion performance in aggressive combustion environments.
IN792’s lower chromium is a deliberate sacrifice: strength was purchased at the cost of some environmental resistance. Coatings can bridge part of that gap, but the base-alloy ranking remains.
IN738LC’s wider freezing range meansgreater segregation tendency, a known casting challenge that demands careful solidification control. IN792’s narrower freezing range is more forgiving in this respect, but its higher γ′ content and refractory load still place it among the alloys that are “readily cast or forged” yetdifficult to process by laser powder bed fusion or welding.
Neither alloy is weldable in the ordinary sense. Both sit in the class of high-performance superalloys that resist LPBF and fusion welding because ofhot cracking driven by steep thermal gradients, wide freezing ranges, and γ′-related ductility troughs. The strain-age cracking risk is especially acute whenAl + Ti exceeds roughly 6 wt%, a threshold both alloys cross comfortably.
The nuance lies in the research and processing pathway. IN738LC has the deeper additive-manufacturing literature: crack-mitigation strategies including substrate preconditioning and post-processing routes have been validated on this alloy, and it is routinely used as a benchmark for cracking susceptibility alongside IN718 and IN625. IN792 has also received attention—preventing microcracks between a deposited layer and an IN792 substrate has been demonstrated using an IN625 buffer layer, and laser welding ofdirectionally solidified IN792 DShas produced joints free of macro-defects through optimized parameters and post-weld heat treatment. The distinction is one of accumulated evidence: IN738LC is the more extensively mapped territory for additive and repair work, while IN792 DS shows that directional solidification can meaningfully improve joinability when the processing window is properly defined.
The standard schedules reflect each alloy’s phase stability. IN738LC typically receives asolution treatment around 1120 °C followed by a single age at 845 °C. IN792 generally requires atwo-step age—1080 °C followed by 845 °C—after solutioning, a more elaborate schedule that reflects the need to control the precipitation of a more heavily alloyed γ′ population.
The choice resolves into three duty-driven questions.
If the limiting requirement is elevated-temperature creep strength and γ′ stability, IN792 is the stronger candidate. Its higher Ta and W contents and higher γ′ solvus make it the alloy that can hold microstructure and shape at the upper end of the temperature–stress envelope.
If the service environment carries sulfur- and vanadium-bearing combustion products and the application values a long, mature service record, IN738LC is the safer specification. Its higher chromium delivers demonstrably better hot corrosion resistance, and the low-carbon version adds ductility and fatigue performance on top of that environmental advantage.
If the route involves additive manufacturing or repair welding, neither alloy is a drop-in solution. IN738LC offers the larger body of validated crack-mitigation knowledge; IN792 DS offers evidence that directional solidification plus high-energy-density welding can produce defect-free joints under optimized conditions. The decision should weigh which processing evidence base maps more closely onto the intended component geometry and repair strategy.
IN792 and IN738LC are not competitors so much ascomplements within the same materials strategy. IN792 answers the demand for more temperature and more creep resistance by spending chromium and adding Ta and W. IN738LC answers the demand for corrosion tolerance and proven industrial service by holding chromium high and carbon low. Reading the composition table as a set of trade-offs—rather than a scorecard—is what allows a designer to place each alloy where its strengths are decisive and its limitations are covered by coating, cooling design, or processing control.